Layup is inside 1x 300gsm - 12mm corecell (not 10mm my mistake ) - 450 gsm 0/90 biaxial outside. Boat is a 7.5m sportsboat with lots of internal...
If you tell me what extra info you need........
Laminate is a single layer outer skin over 10mm corecell on a 6m hull, using ampreg 22 resin
Thanks for the replies, will go with the rebate in the foam, I'm guessing 30mm overlap should be enough.
Hi Guys, Just want to know what the minimum overlap on cloth joins I can get away with. Layup is 1 x 450grm 0/90 double bias ( outside skin )...
The application is for a locker under the cockpit floor so uv not an issue. My main concern was the bonding of the two differen't types of resin,...
Can polyester flowcoat be applied over epoxy laminate or am I better off mixing some pigment into the epoxy for a sealing coat?
24hrs at 60 deg C did the trick, all tackiness has gone & laminate bonded to foam well.
Thanks for all the advice, will set up a insulated cover over the hull tomorrow and try heating up & see how that goes first. If we have to cut...
Gonzo, won't be able to remove with scraper & torch as corecell would be damaged.
Thanks for the feedback. I'll try some more heat for starters before removing laminate. Rest of layup went off ok just this one area thats not...
I have one area of a inside hull layup that remains slightly tacky weeks later. Temp at time of layup was around 18-20 deg c & have since warmed...